SOP: Thickness of Plastic Film and Sheeting (ASTM D6988)

GIFSQ ID: SOP-0991

Nearly every other number a packaging laboratory reports leans on thickness. Gas transmission resistance rises directly with it, stiffness and other strength properties shift with it, and density itself is derived from dimensions together with mass. A film whose gauge varies across its width can therefore pass one test and fail another for reasons that stay invisible until somebody measures the sheet properly.

Measurement itself is simple: a micrometer, several positions across the specimen, and an honest mean. One trap hides in that simplicity: very thin films fall below what ordinary instruments can resolve, and those need microscopy instead.

Purpose

Purpose is to determine the thickness of plastic film and sheeting specimens and report a representative mean, following ASTM D6988, Standard Guide for Determination of Thickness of Plastic Film Test Specimens.

Scope

Scope covers plastic films and sheeting, including bioplastic films of the kind used in the source example, where mean thicknesses of 78.8 µm for a control soy protein isolate film and 89.5 µm for a polylactic acid film are reported. Checking dimensional accuracy is described in the source as one of the most basic quality control procedures, and thickness feeds costing as well as performance judgement. Films under 1 µm thick move out of micrometer territory and into the microscopy branch below.

Equipment and Materials

  • Micrometer suitable for film thickness measurement
  • Microscope arrangement for microtome-cut sections, for very thin films
  • Scanning electron microscope access, for very thin films where that route is chosen
  • Microtome for preparing cut sections for microscopic measurement
  • Film or sheeting specimens, flat and representative of the material to be reported
  • Record sheet for each reading and its position

Procedure

  1. Define the quantity. Work to the source definition throughout: thickness is the perpendicular distance between the two outer surfaces of the material. Readings taken at an angle, or across a fold or crease, do not measure that distance.
  2. Select the specimen. Take film representative of the roll or batch under test, avoiding damaged areas, as general laboratory practice. Handle it without stretching, since a stretched film is a thinner film.
  3. Measure with the micrometer. Bring the micrometer onto the film and take the thickness reading at the chosen position, following the instrument maker’s operating instructions, as general laboratory practice.
  4. Repeat at different locations. Measure at different locations on the sample rather than relying on a single point; gauge variation across a specimen is exactly what a single reading would hide.
  5. Branch for very thin films. Where film is thinner than 1 µm, measure thickness by microscope on a microtome cut, or by scanning electron microscope, instead of by micrometer. Sensitivity drives this branch: the source cautions that typical micrometers, reading in increments of one ten-thousandth of an inch (0.0001 in.) or even 0.00005 in., are simply not sensitive enough for such work.
  6. Calculate the mean. Average the individual readings to give the mean thickness of the specimen, the figure the source uses for reporting and for feeding into other tests.

Recording Results

Record every individual reading, the locations measured, the instrument used and the calculated mean thickness, in µm or in the inch units of the instrument, stated explicitly. Where thickness feeds another determination, such as a permeability coefficient or a density calculation, report the mean actually used there, so a reader can trace the later result back to these readings. Source example values, 78.8 µm and 89.5 µm for two bioplastic films, are illustrations, not specification limits.

Quality Control

Spread of readings carries as much information as their mean. A wide spread signals uneven gauge, and any later mechanical or barrier result should be read with that unevenness in mind, because stiffness is influenced by thickness and gas transmission resistance increases directly with it. Zero and cleanliness checks on the micrometer before a series, and repeat readings where one value sits far from its neighbours, are the practical controls, applied as general laboratory practice; the sources give no numeric repeatability limit, and none is claimed here.

Troubleshooting

  • Readings scatter more than expected: measure additional locations to characterise the variation rather than discarding awkward values; genuine gauge variation is a finding, not noise.
  • Film reads near or below the micrometer’s useful resolution: change branch; use a microtome cut under the microscope, or a scanning electron microscope, as the source directs for films under 1 µm.
  • Suspected compressed or creased spot: move to an undamaged, flat area and note the exclusion; a crease measures doubled material.
  • Mean disagrees with a supplier’s stated gauge: compare the pattern of locations measured before disputing either value; different patterns on an uneven film can honestly produce different means.

Interferences and Limitations

Surface irregularity, creasing and stretching all distort a reading, and soft films can respond to the measuring instrument itself, so results belong to the method and instrument named in the record. Resolution sets the hard boundary at the thin end, which is why microscopy takes over below 1 µm. Beyond that, the sources describe thickness only briefly: no standardised sampling pattern, contact pressure or conditioning regime is given in them, so laboratories needing those specifics must take them from ASTM D6988 itself, and should record whatever pattern they adopt.

Safety Notes

  • Take care with microtome blades when preparing cut sections: guard the blade, cut away from the hand and dispose of used blades in a sharps container, as general laboratory practice.
  • Follow the scanning electron microscope facility’s own safety and sample-preparation rules where that branch is used, as general laboratory practice.

Source and Standard

Drafted from Chapter 9, section 9.2.1.1, of Food Packaging Materials: Testing & Quality Assurance (Singh, Wani and Langowski, eds., CRC Press, 2017), with the role of ASTM D6988 as the thickness guide for plastic film test specimens confirmed in Chapter 4 of the same book; Chapter 3, section 3.2.2, was also read and contains no thickness procedure. Governing standard: ASTM D6988, Standard Guide for Determination of Thickness of Plastic Film Test Specimens.