SOP: Vertical Load (Axial Crush) Strength of Glass Containers
GIFSQ ID: SOP-0982
Glass carries weight far better than it takes a blow. Stacked cases, a pallet load above them, and capping machinery pressing down on a finish all load a container along its axis, and glass under purely compressive force resists a surprising amount of it. Failure, when it comes, is rarely about wall thickness alone: shape decides where stress gathers, and in most designs a shoulder region carries highest stress.
Vertical load testing puts that resistance on a compression tester. Results are read against shape first of all. Source material makes a point worth keeping in front of any user: lightweight nonreturnable bottles of a well-shaped design can match heavier reusable bottles of similar design, because shoulder geometry matters more than glass weight here.
Purpose
Aim is to determine resistance of a glass container to vertical load forces, also called head load, compression or axial load, so designs and production lots can be judged for stacking, capping pressure and other top-down loads in filling, warehousing and distribution.
Scope
Coverage is glass food and beverage containers whose service includes load applied along a vertical axis. Finished product strength is treated in source chapter as among most important physical properties of glass containers. Scope does not extend to internal pressure resistance, impact or thermal shock: each is a separate property with its own test, and a container can perform well in one and poorly in another.
Equipment and Materials
- Compression tester able to apply and measure a vertical, axial load to a container standing on its base
- Flat, stable support for a container base, aligned with loading axis of a tester
- Load recording suitable for capturing maximum load a container bears
- Callipers or gauges for container height, diameter and shoulder form
- Balance for container weight, where weight is part of a comparison
- Protective shielding appropriate to testing glass to failure, plus a brush, scoop and closed container for broken glass
- Labels and a record sheet identifying design, maker or lot, and any surface treatment
Procedure
- Select containers representative of a design or lot. Record design name or shape description for each one: shape is a primary variable, and results cannot be interpreted without it.
- Inspect each container. Note visible damage, scratches or abrasion, annealing or fabrication defects, and coating state, since surface condition and fabrication history influence glass strength.
- Record dimensions and weight where a comparison between designs is intended, including shoulder form and radius of vertical curvature of a shoulder, since source figure plots mean bearable load against that radius.
- Stand a container upright on its bearing surface, centred under loading axis of a compression tester, so load applies vertically and axially.
- Confirm a container is stable and truly upright before loading. A leaning container concentrates load off its axis and produces a failure that belongs to set-up, not glass.
- Apply load with a compression tester, increasing it along a vertical axis. Source text gives no loading rate, so a worksheet must state rate actually used and hold it constant across a comparison set.
- Continue until a container reaches its bearable limit and fails, or until a predetermined examination load fixed outside this SOP by a specification is reached. Source text defines no individual pass load, so do not treat shape averages below as acceptance limits for a single container.
- Record maximum load borne, in kilograms as source figure expresses it, noting where failure originated where that can be seen, in particular whether breakage began in a shoulder region.
- Clear broken glass completely from a tester before mounting a next container, and inspect surfaces for fragments that could point-load a following specimen.
- Repeat on further containers of same design as a laboratory sampling plan requires. Source text gives no specimen count, so number tested must come from that plan and be stated in a report.
Recording Results
Report load borne by each container individually, and a mean bearable load for a design where several containers were tested, expressed in kg. Always report shape beside a mean. Source values, given as average bearable loads by shape, are: champagne shape, 5000 kg; shoulder shape, 4000 kg; square shoulder, 2500 kg; and Winchester shape, 2000 kg. Source figure plots same relationship against radius of vertical curvature of a shoulder, in mm, to 75 mm. Those figures are comparative reference values, not specifications for accepting an individual container, and a report should say so when quoting them.
Quality Control
- Verify alignment before a run: container, base support and loading axis must share one vertical line.
- Check tester load readings against a suitable reference device under a laboratory calibration programme, as ordinary laboratory practice.
- Compare like with like. Means pooled across shoulder shapes hide a variable source text identifies as decisive.
- Inspect tester surfaces between specimens: a trapped fragment under a base can fail a sound container at a misleadingly low load.
- Record surface treatment for each lot, since containers are often surface-coated to preserve strength and reduce scratching.
Troubleshooting
- Failure at an unexpectedly low load: examine alignment, then base seating, then a container for scratches, damage or fabrication defects.
- Breakage starting at a shoulder: treat as a design signal. Source text places highest stress in a shoulder region in most designs.
- Wide scatter within one design: look for mixed moulds, variable surface condition or handling damage, and separate results by mould or lot where records allow.
- Heavier containers performing no better than lighter ones: do not assume an error. Source text states glass thickness is not important in comparison with bottle shape, especially shoulder design.
Interferences and Limitations
Shape dominates this measurement, so a vertical load value travels poorly between designs. Shoulder design in particular governs where stress concentrates. Surface damage, abrasion, annealing faults and fabrication defects can lower what a container bears without any change in nominal dimensions. A test also addresses one force direction only: a container strong axially may still be vulnerable to internal pressure, impact or thermal shock. Finally, source description is short. Loading rate, specimen numbers, container preparation and an individual acceptance load are not given, and comparative shape values should never be promoted into pass or fail limits for production release.
Safety Notes
- Expect sudden, energetic failure. Test glass to failure only behind shielding or in an enclosed tester, with eye protection, following ordinary laboratory practice.
- Keep hands out of a loading zone while a tester is powered, and isolate it before clearing fragments.
- Pick up broken glass with a brush and scoop, never bare hands, and place it into a closed, puncture-resistant container.
- Stop a test if a container shifts or tilts under load: an eccentrically loaded container can eject fragments sideways.
Source and Standard
Method follows Chapter 6, section 6.4.2, of Food Packaging Materials: Testing & Quality Assurance (CRC Press, 2017), by Gul, Wani, Singh, Wani and Wani, including its shape comparison values and its figure relating mean bearable load to radius of vertical curvature of a shoulder. Source section names no standard number for vertical load testing, so none is cited here.