Login Register

Access the GIFSQ Portal

Select your user type to log in or register a new account.

Student Portal

Access your food safety courses and exams.

Instructor Portal

Manage courses, view student submissions, and grade quizzes.

Company Portal

Manage corporate setup, view employee logs, and access QA services.

SOP: Melt Flow Rate (MFR) of Thermoplastics (ISO 1133 / ASTM D1238)

GIFSQ ID: SOP-0986

Few numbers travel with a packaging resin as widely as its melt flow figure. Converters quote it on purchase specifications, and quality teams reach for it first when a film or container suddenly runs differently on a line. Behind that single value sits a deliberately simple idea: push molten polymer through a standardised capillary under a fixed load at a fixed temperature, then measure how much material emerges in a set time.

Simplicity is both strength and weakness here. A melt index result speaks clearly about lot-to-lot uniformity and helps separate one grade from another, yet it captures flow at just one shear stress and one temperature. Anyone needing a full viscosity picture should pair this test with capillary or parallel-plate rheometry rather than stretching a single-point result further than it can go.

Purpose

Aim of this procedure is to determine melt flow rate, reported in grams per 10 minutes, for thermoplastic packaging polymers and bioplastics, and to use that value to check flow uniformity, distinguish grades, and flag material whose flow behaviour has shifted. Guidance on melt volume rate is included only to the extent flagged in the opening note: volume-based reporting follows the same extrusion principle, but the source book gives no separate MVR definition or formula, so no MVR calculation is stated in this SOP.

Scope

Coverage extends to thermoplastics, including bioplastic grades, in a form that can be loaded into a heated extrusion plastometer barrel. Both manual cut-and-weigh working and an alternative timed piston-travel approach for high-flow materials are covered, exactly as the source describes them. Materials that degrade or crosslink at their test temperature fall outside scope. Results allow rough comparison of flow between materials and grades; they do not, on their own, predict behaviour in large-scale processing.

Equipment and Materials

  • Extrusion plastometer (melt indexer): heated cylinder or barrel, piston, standard capillary die of specified length and diameter, and a set of specified dead weights for loading the piston
  • Temperature control and indication for the barrel, capable of holding the specified test temperature steadily through a run
  • Balance suitable for weighing extrudate cuts
  • Timer or stopwatch for cut intervals and, for the piston-travel variant, an electrical or mechanical device that times piston travel automatically
  • Cutting tool for taking extrudate cuts cleanly at timed intervals
  • Charging tool for introducing material into the barrel from the top and settling it on the piston
  • Cleaning tools and materials for the barrel, piston and die, used between materials
  • Test material, identified by polymer, grade and lot, plus its melt density at test temperature where the piston-travel calculation is to be used
  • Current editions of ISO 1133 and ASTM D1238, consulted for the prescribed temperature, load, die dimensions and timing that apply to the polymer under test

Procedure

  1. Select test conditions before touching the instrument. Take barrel temperature, applied load, die dimensions and cut timing from ISO 1133 or ASTM D1238 for the named polymer and grade. Record which standard and which condition set was chosen, because a melt flow value has no meaning divorced from its temperature and load.
  2. Preheat the apparatus to the specified temperature and allow it to stabilise. Confirm the barrel is clean, with piston and die free of residue from any earlier material.
  3. Charge material into the cylinder from the top. Settle it so voids are minimised, then place the piston in position.
  4. Apply the specified weight on the piston. Applied load drives molten polymer downward through the die as the charge melts and reaches test temperature.
  5. Allow flow to establish, then discard the initial extrudate. Early material may carry air bubbles and contaminants, so it never forms part of a measured cut.
  6. Take cuts for the test at timed intervals suited to the material and its flow rate. Slow-flowing grades need longer intervals between cuts; fast-flowing grades need shorter ones, chosen under the governing standard so each cut can be handled and weighed reliably.
  7. Weigh each cut promptly and note the interval over which it was collected. Keep cuts separate until weighing is finished, so a suspect cut can be identified and set aside.
  8. Calculate melt index for each cut and express the result in grams per 10 minutes, following the recording rules below. Report a run value in line with the governing standard, together with temperature and load used.
  9. For a material with a high flow rate, use the alternative timed approach instead of cut-and-weigh where the instrument provides it. Time piston travel automatically, by an electrical or mechanical device, over a calibrated length of travel, then calculate flow rate from piston travel, melt density and time using the formula given under Recording Results.
  10. Empty and clean the barrel, piston and die at the end of a run while the apparatus is still hot enough for residue to be removed. Carry-over contaminates the next material, so leave the instrument clean and ready.

Recording Results

For cut-and-weigh working, convert each weighed cut to a 10-minute basis and report melt index, also called melt flow rate (MFR), in grams per 10 min (g/10 min). Always report alongside a result: polymer and grade, lot identity, test temperature, applied load, standard followed (ISO 1133 or ASTM D1238), and whether cuts were weighed directly or piston travel was timed.

For the timed piston-travel method, calculate flow rate as:

Flow rate = (426 × L × d) / t

where L = length of calibrated piston travel (cm); d = density of resin at test temperature (g/cm3); and t = time of piston travel for length L (s). Melt volume rate (MVR), conventionally expressed in cm3/10 min, is not calculated in this SOP: the source book states no MVR formula, and deriving one here would go beyond the source. Where a customer or specification asks for MVR, obtain it under the current ISO 1133 procedure on an instrument that measures volume displacement directly, and say so on the report rather than converting an MFR value by an unstated route.

Interpretation needs care. Higher melt index means easier flow and, in general, lower material viscosity; lower melt index means stronger resistance to flow. High-molecular-weight material resists flow more than low-molecular-weight material, which is why the test separates grades so usefully. Quote results to a precision consistent with cut weights and timing, and never compare values obtained under different temperatures or loads as though they were interchangeable.

Quality Control

  • Run a material of known, stable melt flow behaviour at intervals set by laboratory practice and after any maintenance, die change or temperature-controller work. Investigate drift before releasing further results.
  • Verify barrel temperature independently at the specified set point before a test series. A small temperature error shifts flow markedly in most thermoplastics.
  • Inspect every die and piston for wear, scoring or partial blockage before use. A damaged die changes flow for every material run through it.
  • Repeat a determination when individual cuts disagree more than laboratory experience with that polymer allows, after checking for bubbles, contamination or an unsteady temperature.
  • Keep charge practice consistent between operators: amount loaded, settling and timing from loading to first cut all influence early flow.

Troubleshooting

  • Bubbles in extrudate: moisture or trapped air in the charge is the usual cause. Dry hygroscopic material as its material standard requires, charge and settle carefully, and keep discarding initial extrudate until a clean, bubble-free strand emerges.
  • Erratic cut weights: check for an unsteady barrel temperature, a partly blocked or dirty die, and inconsistent cut timing. Clean the die, confirm temperature stability, then repeat.
  • Strand will not flow: confirm the correct (heavier) specified load is fitted, the barrel has truly reached the specified temperature, and the die is not blocked with degraded residue.
  • Flow far faster than expected for the grade: suspect a wrong temperature or load, a wrong or worn die, or degradation of the charge from sitting too long in a hot barrel. Stop, verify each condition, and rerun on fresh material.
  • Timed-travel result disagrees with cut-and-weigh: check the melt density value used for that temperature and the calibration of travel length and timer before questioning the material.

Interferences and Limitations

Additives sit at the heart of this test’s main limitation. Plastics are seldom manufactured without additives that affect processing characteristics such as stability and flowability, and their effect is not readily observed through the melt index test. Melt rheology also depends on many variables whose values in a small plastometer may differ substantially from those in large-scale processes, so results may not correlate directly with processing behaviour. Because only one shear stress and one temperature are sampled, shear-thinning across a processing range stays invisible: two materials sharing one melt index can still flow very differently in an extruder or mould. Degradation during long barrel residence, moisture in hygroscopic polymers, and contamination from a previous material each distort results in ways a single number cannot reveal.

Safety Notes

  • Treat barrel, piston, die, weights and fresh extrudate as burn hazards throughout a run and during hot cleaning. Use heat-resistant gloves for charging, cut-taking and cleaning.
  • Handle hot polymer strands and cuts without skin contact, and allow waste extrudate to cool fully before disposal.
  • Take care with heavy dead weights: seat them securely on the piston and lift them with a firm grip to avoid drops onto feet or the instrument.
  • Ventilate as routine laboratory practice requires where a polymer fumes or degrades at test temperature, and remove degraded charges promptly rather than leaving them to break down in the barrel.
  • Keep cleaning tools dedicated and in good condition, so cleaning a hot barrel never involves improvised implements near the die orifice.

Source and Standard

Procedure above is drawn, in original wording, from Singh, Wani and Langowski (eds.), Food Packaging Materials: Testing & Quality Assurance, CRC Press, 2017: Chapter 9, Section 9.2.5 and 9.2.5.2 (Melt Index Test), and Chapter 3, Section 3.6.2 and 3.6.2.3 (Melt Index), including the piston-travel formula credited there to Shah (2007). Governing standards named in the book and in the SOP title are ISO 1133 and ASTM D1238, Standard Test Method for Melt Flow Rates of Thermoplastics by Extrusion Plastometer. Prescribed temperatures, loads, die dimensions and timing for any given polymer must be taken from the current edition of the chosen standard: the book names the standards but does not reproduce their condition tables, and the book contains no treatment of melt volume rate (MVR) at all.