Login Register

Access the GIFSQ Portal

Select your user type to log in or register a new account.

Student Portal

Access your food safety courses and exams.

Instructor Portal

Manage courses, view student submissions, and grade quizzes.

Company Portal

Manage corporate setup, view employee logs, and access QA services.

SOP: Compression Testing of Transport Packages and Shipping Containers (ASTM D642 / ISO 12048)

GIFSQ ID: SOP-0985

Stacking pays for warehouse space, and the bottom package carries the bill. Loads from warehouse stacking, vehicle stacking, and unit-load handling press down for days or weeks, sometimes at hundreds of pounds force, while clamp trucks add horizontal squeezing during handling. A container that yields does more than look crushed: product breaks, primary packs breach, and a leaning stack can become a safety problem.

Compression testing measures how much load a container, component, or unit load can carry before it deforms or fails, and how it behaves while carrying a sustained load. Two branches answer two different questions. Loading at a constant rate until failure finds ultimate strength. Holding a constant load over time, the stacking route, asks whether the package survives the warehouse, where time, humidity, and alignment steadily erode the strength a short test suggests.

Purpose

Objective is to determine the compressive resistance of shipping containers, components, and unit loads, and to use that information in design and stacking decisions. Constant-rate loading characterises maximum resistance and deformation; constant-load stacking work examines endurance under a chosen load for a chosen period. Laboratory strength is a starting point for a stacking judgement, not the judgement itself.

Scope

Scope includes single shipping containers, container components, and complete unit loads, empty or filled, tested under top-to-bottom compression, with related fibreboard container practice noted in the source. Vertical stacking loads sit at the centre of the procedure; horizontal clamp handling loads are a related distribution hazard but require their own arrangements and are not covered by the platen procedure below. Pallet strength and stiffness testing, in which pallet support conditions strongly influence how loads spread into packages, belongs to companion pallet methods and is likewise outside this SOP.

Equipment and Materials

  • Compression tester sized for the specimen, from bench or floor machines for individual packages up to systems able to test a full unit load, with computer-based control of applied load and documentation of results
  • Fixed platen and swivel (floating) platen options, selected and recorded for each run, since platen behaviour forms part of the test condition
  • Load and deflection measurement through the tester control system, checked before a test series
  • Shipping containers, components, or unit loads prepared exactly as intended for distribution, whether empty or filled
  • Conditioning chamber capable of holding a selected standard atmosphere
  • Measuring equipment for container dimensions and for deformation during and after loading
  • The governing specification or schedule, which sets required loads, hold periods where applicable, and acceptance criteria

Procedure

  1. Set the objective first: ultimate compressive resistance, endurance under a sustained stacking load, or both, and the specimen form: single container, component, or unit load, empty or filled. Industry commonly evaluates single empty containers, but filled, stacked, and unitised packages behave differently, so choose the form matching the decision at hand and state it in the record.
  2. Prepare specimens faithfully. Assemble, fill, close, and, for unit loads, stack and secure specimens exactly as in distribution, including stacking pattern and any stretch wrap or strapping, since securement and pattern change how load is shared among packages.
  3. Condition the specimens. Hold them in the atmosphere selected from ASTM D4332 / ISO 2233 for the storage and transport chain under study before loading. Atmospheres given in the source are: cryogenic, minus 55 plus or minus 3 degrees C; frozen food storage, minus 18 plus or minus 2 degrees C; refrigerated storage, 5 plus or minus 2 degrees C at 85 plus or minus 5 percent relative humidity; temperate high humidity, 20 plus or minus 2 degrees C at 90 plus or minus 5 percent relative humidity; tropical, 40 plus or minus 2 degrees C at 90 plus or minus 5 percent relative humidity; and desert, 60 plus or minus 2 degrees C at 15 plus or minus 2 percent relative humidity. Conditioning is not decoration here: environment, especially high humidity acting on fibre-based materials, can cut real-world compression performance to a quarter or less of laboratory strength, so an unconditioned dry result must never be presented as a warehouse prediction. Record atmosphere and conditioning period for every specimen.
  4. Inspect, measure, and photograph each conditioned specimen. Record dimensions, alignment, and any pre-existing damage or lean.
  5. Centre the specimen between the platens in its normal stacking orientation, with load applied top-to-bottom as it would arrive from packages above. Select fixed or swivel platen operation as the method and specification direct, and note the selection: a fixed platen holds the loading face parallel, while a swivel platen can follow the specimen as it deforms, and results from the two arrangements should not be mixed in one comparison without saying so.
  6. Branch A: constant rate of loading (compression). Apply load at the constant rate required by the governing standard and specification, increasing steadily while load and deflection are recorded. Continue until failure, defined by the governing document, typically seen as yielding, buckling of walls, or collapse, or until a specified maximum load is reached. Capture peak load and the deformation at key points, including at failure.
  7. Branch B: constant load (stacking). Apply the selected stacking load, derived from the governing specification for the intended stack, and hold it constant for the specified period. Watch deflection over time: creep is the behaviour this branch exists to expose, since a container can carry a load briefly and still deform progressively across days of storage. At the end of the hold, release the load as directed and record residual deformation and condition.
  8. Examine the specimen after either branch. Note where deformation or failure began: walls, corners, seams, closures, or the product and primary packs inside. For filled specimens, open and check contents condition rather than judging from the outer container alone.
  9. Judge against criteria set in advance in the governing specification. Where a design stacking load must be inferred from a constant-rate result, apply whatever safety or environmental allowances the specification requires and show that working openly in the report; allowances for time under load, atmosphere, alignment, and unitisation belong to the specification, not to habit.

Recording Results

Record specimen identification and form, packing or unit-load configuration, conditioning atmosphere and duration, platen type used, and branch run. For constant-rate work, report the load and deflection record, peak or failure load, deformation at failure, and failure location and mode. For constant-load work, report the applied load, hold duration, deflection against time, residual deformation, and end condition. Photographs before, during where practical, and after loading anchor the numbers. Always state which loads, rates, and durations came from the governing standard or specification, since the source book does not tabulate them and a reader must be able to trace each value.

Quality Control

Check load measurement and platen condition before a series, and keep preparation, orientation, and conditioning consistent across any set meant to be compared. Replicate testing deserves emphasis because container strength varies with material lots, converting, and humidity history. Interpretation needs equal discipline: research summarised in the source shows systematic differences between stacked and unstacked, unitised and non-unitised, and filled and unfilled performance, plus a strong influence from pallet stiffness on how stress distributes through a load. A single-container result quoted without those qualifiers invites overconfidence. Confirm important stacking decisions against real stored loads where possible.

Troubleshooting

  • Specimen leans or load lands unevenly: stop, check centring, container squareness, and platen selection; an off-centre start manufactures a failure the design never earned.
  • Failure at a seam or closure only: examine assembly and closing practice before condemning the container design; converting and closing variation frequently governs the result.
  • Strong constant-rate result, poor stacking endurance: treat creep and atmosphere as prime suspects; review conditioning, hold load derivation, and storage humidity rather than repeating the short test.
  • Wide scatter between replicates: review material variation, moisture history, and specimen preparation consistency, and increase replication before drawing design conclusions.

Interferences and Limitations

Time is the quiet variable: strength measured over minutes overstates resistance over weeks. Atmosphere compounds that effect, alignment in a real stack is rarely perfect, and packages interact with pallets and neighbours in ways a single-container test cannot capture. Empty-container results do not automatically describe filled behaviour, since contents may either support walls or transmit load to vulnerable points. Horizontal clamp loads and dynamic handling loads fall outside a vertical platen result entirely. Within those limits, compression data remain the soundest basis available for comparing designs and informing stacking practice.

Safety Notes

  • Stand clear of the specimen under load; containers and unit loads can collapse suddenly and eject contents or fragments.
  • Never reach between platens while the tester is powered or a load is applied, and follow the tester lockout procedure for clearing a collapsed specimen.
  • Use mechanical handling for unit loads and heavy containers during loading and removal.
  • Take care with broken glass, damaged pressurised packs, and spilled contents after failure, and follow site rules for conditioning chambers at temperature and humidity extremes.

Source and Standard

This SOP is drawn from Singh, Wani and Langowski (eds.), Food Packaging Materials: Testing and Quality Assurance (CRC Press, 2017), Chapter 4, Section 4.4.3 and Chapter 10, Sections 10.3.3 and 10.3.8.3. Named standards are ASTM D642, Standard Test Method for Determining Compressive Resistance of Shipping Containers, Components, and Unit Loads, and ISO 12048, Packaging: Complete, Filled Transport Packages: Compression and Stacking Tests using a Compression Tester, with TAPPI/ANSI T804 for fibreboard shipping containers also noted in the source, and conditioning per ASTM D4332 and ISO 2233. Consult the current standards and the product specification for loading rates, stacking loads, hold periods, and acceptance limits.