Physical Analysis
SOP: Determination of Tear Resistance (Elmendorf Test)
Principle Tear strength, reported in grams, is the force necessary to continue tearing a sample after a nick has been made. In the Elmendorf tear tester, a sample is clamped to a pendulum and nicked; on release, the pendulum tears the specimen, and the scale registers the arc through which the pendulum swings. The arc […]
SOP: Determination of Bursting Strength (Mullen Test)
Principle Bursting strength is the hydrostatic pressure required to rupture the material: pressure is applied at an increasing rate through a rubber diaphragm to a circular area 1.2 inch in diameter. The material under test is initially flat and held rigidly at the circumference but free to bulge as the pressure rises. The test is […]
SOP: Determination of Tensile Strength and Elongation of Packaging Materials
Principle Tensile strength is a fundamental property indicative of the serviceability of a packaging material: it determines the resistance to rupture when the material is subjected to a pulling force. Elongation, measured on the same machine, is the extent to which a material will stretch before breaking; a large elongation indicates toughness, since the material […]
SOP: Determination of Gas Transmission Rate of Films
Principle The test film is clamped to a gas transmission cell; test gas is admitted to one side of the specimen while the other side is evacuated. The gas permeates through the film into the evacuated chamber over a measured length of time, and the gas transmission rate is calculated from the geometry of the […]
SOP: Determination of Water Vapour Permeability by the Cycle Method
Principle The cycle method tests the water vapour permeability of finished packages subjected to extremes of temperature and relative humidity when closed and sealed in the conventional manner. It is intended for shelf-size packages that are shipped in outside containers. The sealed package is cycled between a low-temperature room and a high-temperature, high-humidity chamber, and […]
SOP: Determination of Water Vapour Permeability of Packages by the Package Method
Principle The water vapour permeability of a finished package is determined as the rate at which water is transmitted into the sealed package from the test atmosphere (normally 90 ± 2% RH at 37.8 ± 1°C) surrounding it, while a desiccant or the product itself is sealed within. The desiccant version measures the permeability of […]
SOP: Determination of Water Vapour Transmission Rate by the Dish Method
Principle The water vapour transmission rate (WVTR) of a packaging material is measured by the dish method: an open dish filled with desiccant is tightly covered with the test specimen and exposed to a controlled temperature and humidity. The desiccant gains weight as water vapour permeates through the specimen, and the steady-state rate of weight […]
SOP: Conditioning of Paper and Paper Products for Testing
Principle Paper and paper products change their moisture content with the surrounding atmosphere, and their measured strength and permeability values depend on that moisture content. Test results are therefore only comparable when specimens are brought to a standard conditioned state before testing: a circulating atmosphere held at 65 ± 2% relative humidity and 27 ± […]
SOP: Dimensional Checking of Glass Containers
Principle Dimensional checking ensures that the bottle will perform satisfactorily during filling, packing and handling. The bottle height is measured with vernier instruments and the diameter is checked with ring gauges against maximum and minimum limits. Deviation often occurs in local areas of the bottle surface that are not fully blown up to the mould […]
SOP: Measurement of Verticality of Glass Containers
Principle In a cylindrical bottle, the centre of the finish is intended to lie in the vertical plane through the joining faces of the body mould, vertically above the centre of the base. The horizontal distance by which the finish departs from this position is the non-verticality (sometimes called verticality or obliquity). It is measured […]
SOP: Determination of Alkalinity of Glass by the Crushed Glass Method
Principle The quality of the glass itself is determined using powdered glass prepared from the bottles. Alkalinity extracted from the powdered glass into water is titrated with 0.01 N HCl using methyl red indicator. Two procedures are given: a reflux extraction (Procedure A) and a more severe autoclave extraction (Procedure B). Apparatus required Crushing equipment […]
SOP: Determination of Alkalinity of Glass Bottles Using Whole Containers
Principle Glass is attacked by water, and the attack accelerates when repeated high-temperature sterilization (100–120 °C) of filled bottles is carried out. Alkali extracted from the glass changes the colour of methyl red indicator solution. In the whole-container test, the bottle is filled with acidified methyl red solution and autoclaved; a change from pink to […]
SOP: Test for Internal Pressure Resistance of Glass Containers
Principle The resistance of a glass container to internal pressure is tested by filling the bottle with water and applying pressure with a pump, a direct ram, or in a hydrostatic pressure tester. The pressure resistance is proportional to the wall thickness and inversely proportional to the bottle diameter. The wall thickness can be estimated […]
SOP: Tests for Impact Breakage Resistance of Glass Containers
Principle Glass containers break by active impact or by a series of small impacts. The resistance of the bottle to impact is tested either by dropping it from progressively greater heights onto a rigid surface or by striking it with a rigid pendulum whose fall height measures the impact energy. Apparatus required Rigid flat surface […]
SOP: Test for Thermal Shock Resistance of Glass Containers
Principle Thermal shock resistance is measured as the difference between the upper temperature (T₁) of the hot bath in which the containers are heated and the lower temperature (T₂) of the cold water bath into which they are transferred. The containers are examined for cracks or damage after the sudden temperature change. Apparatus required Hot […]
SOP: Determination of Capacity of Glass Containers
Principle The capacity of a glass bottle is defined either as the brimful capacity or as the capacity to a stated filling height. A bottle is brimful when, standing on a level surface, it is filled with water until the centre of the water surface is level with the top of the bottle. Capacity is […]
SOP: Examination of Double Seam
Principle A sound end seam rests on two things: the two hooks interlocking cleanly during seaming, and a thin film of lining compound sealing them. A poor seam can let air leak out or cooling water leak in: and with it, spoilage organisms. The seam is checked visually, measured externally with a seam checking gauge […]
SOP: Performance Test for Tinplate Containers by Test Packs
Principle Lab tests on plate and lacquer are only screening. The real verdict on acid and sulphur resistance comes from packed food: the candidate plate is canned up alongside a plate of known good performance and the two are compared over storage. A plate passes if it performs no worse than a standard plate in […]
SOP: Lacquer Adhesion Test (Scotch Tape Test)
Principle The truest adhesion check is to stamp can ends from the lacquered sheet and look at them. In the laboratory the scotch-tape method stands in: the lacquer is scratched with a fine needle, tape is pressed on, and ripped off. It reliably catches poor adhesion, though it cannot always separate good from middling. Apparatus […]
SOP: Determination of Tin Crystal Size by Acid Etching
How a tin coating’s grain size sits relates to how it corrodes in some media: grain coarser than No. 9 (ASTM) is judged satisfactory. Grain is seen either under polarized light on the untouched surface or after a simple acid etch; the etching bath below brings the crystal pattern out clearly. Purpose To determine the […]
SOP: Tensile Test for Tinplate
Principle The tensile test probes the steel base by pulling a standard strip until it breaks and plotting the load–extension curve. Because the test demands both skill and time to make reproducible, it is rarely run: though it would tell a great deal about the steel’s mechanical properties. Apparatus required Ordinary or “hard-beam” type tensile […]
SOP: Cupping Test for Tinplate (Erichsen and Olsen)
Principle Seamless containers: oval fish cans, screw caps and the like: are made by drawing tinplate. A hemispherical punch drives the specimen into a die to form a cup; the cupping value is how deep the impression has gone when the cup wall first fractures (alternatively, the drop in punch load at the first sign […]
SOP: Jenkins Bend Test for Tinplate
Principle Forming can bodies and flanging ends bends tinplate hard. A strip is gripped between rounded jaws and bent back and forth through a 180° arc until it starts to break. Two strips are tested every time: one along the rolling direction, one across it. Both the gap between the two readings and the level […]
SOP: Determination of Indentation Hardness of Tinplate (Rockwell Test)
Principle Tinplate must survive bending, spinning and drawing during can fabrication without failing. Its hardness is gauged by driving a 1/16-inch steel ball into the plate under a standard load and measuring how deep it goes: the reading rests on the difference between two penetration depths. Apparatus required “Superficial” Rockwell hardness testing machine Suitable anvil […]