SOP: Water Absorptiveness of Paper and Board (Cobb Test) (ISO 535 / TAPPI T 441)
GIFSQ ID: SOP-0981
Paper drinks. Cellulose fibres carry hydroxyl sites and a sheet is a porous network, so board in contact with water pulls that water in, loses stiffness, and passes moisture toward food it was meant to protect. Sizing and coating exist largely to slow that uptake.
Water absorptiveness testing answers with a timed exposure. One face of a weighed test piece, over a defined area, meets a shallow column of water for half an hour. A second weighing after blotting shows what stayed in a sheet, and difference over area exposed gives a value in grams per square metre.
Purpose
Aim is to determine mass of water absorbed by a specified side and a specified area of a paper, board or corrugated fibreboard test piece during a fixed exposure, so materials and surface treatments can be compared for duties where wet contact is expected.
Scope
Coverage in source text extends to paper packaging material generally, with a procedure written around a corrugated fibreboard test piece. Apply it to a face nominated for testing: a side expected to face moisture in service. Results describe that side and area only, since a coated or sized face can behave quite differently from its reverse.
Equipment and Materials
- Cylindrical tank that can be applied to a test piece and hold water over a specified area, with a known nominal cross-sectional area
- Balance for weighing test pieces before and immediately after exposure
- Water for forming a column over a test area
- Blotting paper for treating a tested area after exposure
- Metal roller for rolling a tested area once forward and once backward
- Timer able to control a 30 minute exposure
- Cutting equipment for taking test pieces from undamaged areas
- Conditioning space able to hold a standard atmosphere until specimens reach equilibrium
- Labels and a record sheet noting which side of each piece was tested
Procedure
- Condition material first. Bring specimens into equilibrium with a standard atmosphere before cutting and weighing, following handling source chapter sets for paper specimens generally. Source text for this test gives no numeric temperature or humidity values for that atmosphere, so record actual laboratory conditions beside results.
- Take test pieces from undamaged areas of samples. Avoid creased or crushed material, since damage opens paths for water that a sound sheet would not offer.
- Mark each piece so its specified side can be identified, and weigh it. Record mass before exposure as m1, in grams.
- Apply a cylindrical tank to a specified side of a test piece, over a specified area, so water contacts only that area.
- Pour water into a tank to form a head of at least 3 mm of water upon a test area.
- Leave water in contact for 30 minutes, timing from exposure of a test area.
- Pour water out quickly at end of exposure and remove a tank without delay.
- Place blotting paper on a tested area straight away.
- Roll a metal roller once forward and once backward over blotting paper, with its axis parallel to flutes where a test piece is corrugated fibreboard.
- Weigh a test piece immediately after exposure and blotting. Record mass as m2, in grams.
- Repeat on further test pieces as a laboratory sampling plan requires, keeping side tested and exposure identical across a set.
Recording Results
Calculate water absorptiveness A for each test piece, to nearest g/m2, from:
A = (m2 − m1) / S
Here m1 is mass of a test piece before exposure to water, in g; m2 is mass after exposure, in g; and S is nominal cross-sectional area of a cylindrical tank, in m2. Report a value for each piece along with side tested, rather than a mean alone. Source text gives no numeric tank area, so S must be taken from actual tank in use and stated in a record.
Quality Control
- Check a tank seals against a test piece before pouring: water escaping sideways shrinks area actually exposed.
- Confirm water head reaches at least 3 mm across a whole test area at start of exposure.
- Weigh promptly at both stages. A piece left standing after blotting keeps exchanging moisture with room air.
- Use fresh blotting paper for each piece, and give a roller one forward and one backward pass only.
Troubleshooting
- Very high value on one piece only: inspect for damage, a tank leak, or exposure of a wrong side, then retest a fresh piece.
- Water outside a tank outline: discard that result. Tank seating, not absorptiveness, has governed uptake.
- Values drift across a day: look at conditioning and at delays between draining, blotting and weighing.
- Odd corrugated results: confirm a roller travelled with its axis parallel to flutes, as source procedure directs.
Interferences and Limitations
Surface condition dominates this measurement. Sizing, coating, waxing, lamination or print on a tested face changes uptake, and a result says nothing about an untested reverse face. Damage has a similar effect, which is why pieces come from undamaged areas. A single fixed contact, 30 minutes under a shallow head, does not predict prolonged immersion, hot liquid or pressure behaviour. Source text gives no water temperature, roller mass or numeric test area, so confirm those points match before treating small differences between laboratories as real.
Safety Notes
- Wipe up spilled water promptly: wet floors near balances are a slip hazard.
- Keep fingers out of a roller path across a test piece.
- Take care with cutting tools and with sharp edges on heavier board.
Source and Standard
Method follows Chapter 8, section 8.3.19, of Food Packaging Materials: Testing & Quality Assurance (CRC Press, 2017), by Mir, Wani, Wani, Singh and Wani, including its 30 minute exposure, minimum 3 mm water head, blotting and roller treatment, and its calculation. Water absorptiveness by this Cobb approach is standardised as ISO 535 and TAPPI T 441, which govern test area, water and roller details that source section leaves unspecified.