SOP: Impact Resistance of Plastic Film by Free-Falling Dart (ASTM D1709 / ISO 7765)

GIFSQ ID: SOP-0972

A filled bag dropped off a pallet, a pouch knocked onto a hard floor, a film struck by something falling into it: packaging film meets sudden blows far more often than slow pulls. Impact resistance captures that toughness. Chapter 4 frames impact strength as the force a material needs to resist the penetrating power of a rounded probe under a conditioned test practice, which is exactly what a falling rounded dart delivers to a clamped sheet of film.

Free-falling dart testing turns that idea into a practical comparison. Film is held flat, a dart of known mass falls on it from a set height, and the outcome for each drop is bluntly binary: the film either breaks or it holds. Working up and down through a series of dart masses homes in on the weight at which half the specimens fail, a single figure that separates tough films from brittle ones very effectively.

Purpose

Purpose is to determine the impact resistance of plastic film by the free-falling dart method, expressed through the dart mass at which film specimens fail under the staircase procedure, so films can be compared for resistance to sudden impact and penetration.

Scope

Scope covers plastic film tested under ASTM D1709, Standard Test Methods for Impact Resistance of Plastic Film by the Free-Falling Dart Method, and ISO 7765, Plastics Film and Sheeting: Determination of Impact Resistance by the Free Falling Dart Method, Part 1: Staircase Methods. Chapter 4 places the dart method among related impact approaches, including ASTM D4272 for total energy impact of plastic films by dart drop, and points to ASTM D618 for conditioning, ASTM D6988 for thickness determination and ASTM E177 and E691 for precision and interlaboratory practice. This SOP follows the staircase route only.

Equipment and Materials

  • Free-falling dart apparatus conforming to the standard in use, with a rounded-head dart, a set of dart masses, a release mechanism at the drop height set by that standard, and a clamp that holds film flat and taut
  • Plastic film specimens, cut large enough to clamp securely, free of creases, pinholes and edge damage
  • Conditioning chamber or room able to hold 23 ± 2°C and 50 ± 10% relative humidity
  • Thickness measurement following ASTM D6988, Standard Guide for Determination of Thickness of Plastic Film Test Specimens
  • Record sheet capturing, for every drop: dart mass, specimen identity, and outcome recorded as failure or non-failure

Procedure

  1. Condition the test specimens at 23 ± 2°C and 50 ± 10% relative humidity for more than 40 hours before testing, as Chapter 4 specifies for impact specimens, following ASTM D618 practice.
  2. Measure and record film thickness for the material under test, following ASTM D6988, since impact results are only comparable between films whose thickness is known.
  3. Set the apparatus up exactly as the standard in use requires: dart head, drop height and clamping arrangement all follow ASTM D1709 or ISO 7765 Part 1. Chapter 4 names those standards but states none of their settings, so the current standard text is the authority at this step and no value should be carried over from another laboratory’s habit.
  4. Clamp the first specimen flat and free of wrinkles, release the dart from the set height so it strikes the film, and record the outcome: failure where the dart penetrates or breaks the film as the standard defines failure, non-failure where it does not.
  5. Work the staircase. After a failure, step the dart mass down by the fixed increment the standard sets; after a non-failure, step the mass up by that same increment. Use a fresh specimen for every drop, and keep the increment constant through the whole series so the sequence stays a true up-and-down staircase.
  6. Continue dropping until the specimen count required by the standard in use has been completed, recording mass and outcome for every single drop in sequence, not just the turning points.
  7. Discard and replace any specimen that slips in the clamp, is struck off-centre through a mounting fault, or shows a pre-existing defect at the strike point, and note each discarded drop and its reason in the record.

Recording Results

Report the staircase outcome as the dart mass at which 50% of specimens fail, calculated from the recorded sequence of masses and failure or non-failure outcomes by the calculation given in the standard in use. Chapter 4 does not reproduce that calculation, so the formula, the increment and the counting rules must come from the current text of ASTM D1709 or ISO 7765 Part 1 and be cited in the report. Alongside the result, record film identity and thickness, conditioning applied, drop height and dart configuration from the standard, the mass increment used, and the total number of specimens dropped. Impact strength may also be discussed qualitatively as toughness: a higher 50% failure mass means a tougher film under this test. Results from different drop heights, dart heads or increments are not interchangeable and must never be pooled.

Quality Control

  • Keep one reference film of known behaviour and run a staircase on it at intervals: a shift in its 50% failure mass signals apparatus, clamp or conditioning drift.
  • Inspect darts regularly for dents, corrosion and damaged heads, and verify each mass in the set, because a battered dart head concentrates force and quietly lowers every result.
  • Check clamp grip on scrap film before a series: slipping specimens produce false non-failures that corrupt the staircase.
  • Confirm conditioning records for every batch, since impact specimens carry the chapter’s explicit requirement of more than 40 hours at the stated temperature and humidity.

Troubleshooting

  • Failures at very low masses across all films: examine the dart head for damage, confirm the drop height against the standard, and check that specimens were conditioned for the full period.
  • Specimens tearing at the clamp rather than at the strike point: clean the clamp faces, seat the film evenly, and reject those drops as invalid instead of scoring them as failures.
  • Staircase never turns around: the starting mass is far from the film’s failure region, or the increment does not match the standard. Restart the series with a starting mass chosen from a few scouting drops.
  • Wide scatter between repeat series: look for thickness variation across the film roll, mixed conditioning histories, or defects such as gels and pinholes landing at strike points.

Interferences and Limitations

Conditioning history reaches deep into this result: a film tested dry and cold straight off a roll will not behave like the same film after more than 40 hours at 23 ± 2°C and 50 ± 10% relative humidity, which is why the chapter attaches that conditioning to impact specimens. Thickness differences dominate comparisons between different films, so failure mass should be read alongside measured thickness, never alone. Local defects decide individual drops, and the staircase design absorbs that scatter only when increments, specimen counts and the calculation all follow one standard consistently. Dart drop is also a single-impact, rounded-probe event: it ranks toughness for sudden blows, but it does not predict tear propagation, puncture by sharp objects or repeated-impact fatigue.

Safety Notes

  • Treat the raised dart as stored energy: keep hands and head out of the drop path, and never reach under a loaded dart to adjust film.
  • Handle heavy dart masses with both hands and store them racked, so a dropped mass cannot injure feet or damage the dart head.
  • Cut specimens with a guarded blade, and collect failed film promptly so torn sheets do not litter the floor around the apparatus.

Source and Standard

Adapted from Singh, Wani and Langowski, Food Packaging Materials: Testing and Quality Assurance (CRC Press, 2017), Chapter 4, Section 4.3.1.2, “Impact Strength”, which specifies the conditioning quoted here and names ASTM D1709 and ISO 7765 Part 1, Staircase Methods, as the governing standards for impact resistance of plastic film by the free-falling dart method. Apparatus settings and the failure-mass calculation, not stated in that section, must be taken from the current edition of the standard being followed.