SOP: Challenge Testing of Recycled Plastics for Food Contact (Surrogate Contamination)

GIFSQ ID: SOP-0969

Post-consumer plastic can arrive at a recycler carrying traces of whatever a household stored in it last: motor oil, pesticide mixes, solvents and more. A challenge test answers a practical safety question before any of that material goes back into food packaging. Clean polymer is deliberately soiled with a cocktail of model compounds, called surrogates, run through the full recycling process, and then measured stage by stage to see how much of each surrogate survives cleaning, drying and remelting.

Surrogates stand in for thousands of possible real-world contaminants, so picking them well matters more than picking many. Each one represents a corner of volatility and polarity space, plus a toxic metal salt, so that a process which removes all of them has shown something meaningful about compounds it was never tested against.

Purpose

Purpose is to evaluate whether a plastic recycling process cleans deliberately contaminated polymer thoroughly enough for the recycled resin to be used in food-contact packaging, following the surrogate challenge approach set out in the FDA “Points to Consider” framework for recycled plastics.

Scope

Scope covers secondary (physical) recycling of poly(ethylene terephthalate) (PET), worked as flake and as whole bottles, from surrogate contamination through washing, drying and extrusion into sheet. A typical study runs in four phases: Phase I, flake contamination; Phase II, flake analysis and method validation before and after processing; Phase III, a bottle or plaque migration study; and Phase IV, extract analysis and method validation. Phase III may be unnecessary where post-processing flake levels fall below the criterion given under Recording Results. Laminates in which recycled resin sits behind a virgin functional barrier are tested the same way, with migration measured through the food-contact layer.

Equipment and Materials

  • Virgin PET soda-bottle flake, or whole virgin PET bottles with standard closures
  • Surrogate compounds: toluene, chloroform, lindane, benzophenone, tetracosane and copper(II) 2-ethylhexanoate for the pilot cocktail; diazinon, phenyldecane, calcium monomethylarsenate (CMMA) and zinc stearate are named in the source chapters as accepted alternatives for particular classes
  • Heptane as cocktail carrier solvent, and isopropyl alcohol as solvent for the copper surrogate
  • Glass containers, 4 L, and an incubator held at 40°C
  • Steam-jacketed reaction vessel, about 400 L, fitted with a lightning mixer agitator and a bottom screen and drain
  • Okite R28 surfactant, cold tap water, and a basket centrifuge
  • Dryer capable of holding flake at 160°C, and plastic bags with twist ties for dried flake
  • Single-screw extruder (a Haake unit in the pilot study), with optional vacuum at the vent port, and a centrifugal grinder with a 22 mesh screen for whole bottles
  • Trifluoroacetic acid (TFA), heptane for extraction, 0.1 N nitric acid, wrist-action shaker, and a furnace for ashing at 500°C
  • Gas chromatograph with mass selective detector (GC/MS), 30 m × 0.32 mm ID DB-1 column, atomic absorption spectrometer, and stripping anodic voltammetry equipment
  • Arch punch (1.7 cm diameter), chromel wire, glass bead spacers, EPA vials, heptane and 10% ethanol as food-simulating solvents

Procedure

  1. Select the surrogate cocktail so all FDA volatility and polarity classes are represented. In the pilot recycling study the cocktail held toluene (10%, volatile, non-polar), chloroform (10%, volatile, polar), lindane (1%, non-volatile, non-polar), benzophenone (1%, non-volatile, polar), copper(II) 2-ethylhexanoate (1%, heavy metal) and tetracosane (1%, a second non-volatile, non-polar surrogate of extremely low volatility), dissolved in heptane. Keep every surrogate at or below 10% of the cocktail to minimise solvation of the polymer; heptane made up about 66% by volume and was not itself monitored, screening having shown minimal interaction with PET.
  2. Contaminate the flake. Pack flaked virgin PET, in batches of 100 to 200 kg overall, into 4 L glass containers at 1600 to 1800 g per container and fill with surrogate solution to within 5 cm of the top polymer level. Incubate for 2 weeks at 40°C; thermal expansion of the solution during incubation covers the remaining polymer.
  3. As an alternative contamination route, fill whole virgin PET bottles with 2 L of surrogate solution, cap with standard closures, and incubate for 2 weeks at 40°C. A further example design in Chapter 10 immerses resin in a neat cocktail of chloroform (49.5% by weight), toluene (49.5%), lindane (0.5%) and CMMA (0.5%) for 2 weeks at 40°C with periodic agitation, then drains the cocktail off and air-dries the resin.
  4. Take a sample of contaminated flake for analysis before cleaning begins, so later stages can be compared against the starting load.
  5. Wash the flake. Pour the PET and surrogate slurry into the steam-jacketed vessel and let it drain for 30 minutes through the bottom screen. Close the drain, fill with cold tap water to about 6 cm above the polymer surface (about 150 to 240 L), and add Okite R28 surfactant to a final concentration of 1.5%.
  6. Heat the slurry to 92°C over about 15 minutes, hold at 92°C for 15 minutes, then drain. Allow a 15 minute drainage period, close the drain, and refill with cold water to about 6 cm above the flake surface.
  7. Suspend the flake in the rinse water with the mixer for 15 minutes, reopen the drain, and let the water drain for 15 minutes.
  8. Remove flake manually in batches of about 11 to 14 kg and spin each batch in the basket centrifuge to remove bulk water. Wash whole bottles the same way, submerging floaters so they fill with wash solution, then drain each bottle and grind in a centrifugal grinder over a 22 mesh screen.
  9. Dry centrifuged flake for 4 hours at 160°C. Transfer dried flake at once into plastic bags closed with a twist tie, so moisture is not reabsorbed. Avoid recirculated drying air and desiccant beds in experimental work, because desorbed volatile surrogates saturate recirculated air and distort drying losses.
  10. Extrude the dried flake into sheet of 25 mil ± 2 mil, running the extruder either with vacuum at the vent port (15 ± 1 inHg absolute in the pilot study) or without vacuum, according to the process variant under evaluation. Sample the extruded sheet for residual analysis.
  11. Measure total surrogate uptake and residuals by total dissolution. Treat 2 ± 0.001 g of polymer with 15 mL of trifluoroacetic acid and agitate on a wrist-action shaker until the flake has fully dissolved. Extract the digest three times with 15 mL of heptane, wash the combined extract twice with 10 mL of water to remove residual acid, collect the heptane layer, and dilute to 50 mL with neat heptane.
  12. Analyse 1 µL of the heptane solution by GC/MS, using selected ion monitoring, with all tests performed in triplicate. Determine copper(II) 2-ethylhexanoate separately: ash the polymer at 500°C until carbonaceous matter is removed, dissolve the light ash in 0.1 N nitric acid, and quantify copper by atomic absorption where residuals exceed 0.5 ppm, or by stripping anodic voltammetry below 0.5 ppm.
  13. Run the food-simulating solvent extraction on extruded sheet. Punch disks 1.7 cm in diameter, string 25 disks on chromel wire with glass bead spacers, and place the string in an EPA vial filled to a bulging meniscus with either heptane (fatty simulant) or 10% ethanol (aqueous simulant). Sample at 2, 24, 96 and 240 hours and examine by GC/MS, in triplicate.
  14. Where a full migration study is run, expose finished bottles or plaques to food simulants at 40°C for 30 days, sampling at 1, 3, 10 and 30 days; typically only the day 10 and day 30 samples are analysed.

Recording Results

Record residual concentration for every surrogate at each stage: contaminated, washed, dried and extruded. Cleaning performance is read from that stage-by-stage fall in concentration, surrogate by surrogate, rather than from any single summary figure. Report GC/MS results in ppm for polymer and in ppb for simulant extracts, with triplicate values and their spread; between-study variability in the pilot work was large, reaching a relative standard error of ±100% for volatile uptake and ±400% for non-volatile uptake, so single runs should never be reported without replication.

Judge the outcome against the dietary criterion worked through in Chapter 10. FDA’s threshold approach treats a dietary concentration below 0.5 ppb as negligible risk for a non-carcinogen. Using a consumption factor of 5% for PET, a PET mass to surface area of 0.46 g/in² and 10 g of food per in² of surface, 0.5 ppb in the diet corresponds to 10 ppb in food, which corresponds to a maximum of 217 ppb contamination in the flake. Where post-processing flake holds less than 217 ppb, migration testing may not be required. Dietary estimates in Chapter 9 also apply FDA’s assumption that only 50% of the recycle stream is contaminated with a single contaminant, together with a PET consumption factor of 0.05; on that basis the pilot resin imparted less than 0.5 ppb of all surrogates in aqueous food contact, while fatty-simulant extraction exceeded the 0.5 ppb threshold, so that resin was judged unsuitable for fatty foods.

Quality Control

  • Validate analytical methods by standard additions and recovery calculations at one-half, one and two times the amount detected; where a surrogate is not detected, validate at the limit of detection.
  • Acceptable recoveries under the FDA recommendations quoted in Chapter 10 are 60 to 110% below 100 ppb and 80 to 110% above 100 ppb.
  • Run polymer analyses in triplicate at every stage, and investigate any stage where a residual rises instead of falling: Chapter 10’s first example study showed chloroform unchanged by processing, a result that must be reported as found, not averaged away.
  • Record flake source, flake size and cocktail lot for every run, since uncontrolled differences in PET manufacturer and flake size were likely responsible for much of the between-study variation in the pilot work.

Troubleshooting

  • Measured uptake far above diffusion predictions: check for capillary adsorption on grinder-damaged flake. Cracks, stress fissures and feathered edges act as sinks that trap surrogate, and a waxy film precipitated during cold-water washing can cement trapped surrogate inside those features. Whole-bottle contamination gives far lower uptake than flake for the same cocktail, which points to surface damage rather than bulk absorption.
  • Volatile surrogates barely fall during drying: confirm drying air is not being recirculated through a desiccant bed, which saturates with desorbed volatiles and blunts further loss.
  • Poor replication for non-volatiles: expect wide scatter for compounds such as tetracosane and the copper salt, mix samples thoroughly before subsampling, and keep the 2 g analytical portion representative of the batch.
  • Sheet seals or bags take up moisture after drying: bag dried flake immediately and close it at once, as the pilot procedure specifies.

Interferences and Limitations

Mathematical diffusion models underpredicted surrogate uptake badly in the pilot work, by several thousand-fold for non-volatile compounds, largely because surface-retained surrogate is not Fickian bulk absorption. Models described food-simulant extraction from extruded sheet much better, once surrogates had been mixed impartially through the polymer by extrusion. Aqueous simulants complicate interpretation for non-polar compounds because solubility and partition effects are not captured by the absorption equation, which tends to predict the maximum possible extraction. Surrogate behaviour also shifts with flake crystallinity, which ranges from near zero to about 50% in bottle flake, so results from one feedstock lot do not transfer automatically to another.

Safety Notes

  • Chloroform, toluene, lindane and the other cocktail components are hazardous chemicals: handle the cocktail, contaminated flake and TFA digests in a fume hood with suitable gloves and eye protection, following each compound’s safety data sheet.
  • Trifluoroacetic acid is corrosive, and the 500°C ashing step, the 160°C dryer, the 92°C wash water and the extruder all present burn hazards: use heat-resistant gloves and allow vessels to drain and cool as the procedure directs.
  • Choosing less toxic alternative surrogates where the chapters allow them, such as benzophenone in place of diazinon, raises operator safety without weakening the class coverage of the cocktail.
  • Dispose of surrogate solutions, heptane extracts and contaminated polymer as chemical waste, never as general laboratory refuse.

Source and Standard

Adapted from Risch (ed.), Food Packaging: Testing Methods and Applications (ACS Symposium Series 753, American Chemical Society, 2000), Chapter 9 by Sadler, Hussaini and Pierce on pilot R-PET recycling studies and Chapter 10 by Pesselman and McCort-Tipton on experimental approaches to regulatory compliance for recycled plastics. Both chapters build on the FDA “Points to Consider for the Use of Recycled Plastics in Food Packaging: Chemistry Considerations” (1992) and the 0.5 ppb threshold of regulation approach.